型號 | 截面尺寸(mm) | 理論重量,kg/m | |||
高度H | 寬度B | 腹板厚度t1 | 翼緣厚度t2 | ||
H250×250 | 250 | 250 | 9 | 14 | 71.8 |
H300×300 | 300 | 300 | 10 | 15 | 93.0 |
H350×350 | 350 | 350 | 12 | 19 | 134.9 |
H340×250 | 340 | 250 | 9 | 14 | 78.1 |
H390×300 | 390 | 300 | 10 | 16 | 104.6 |
H440×300 | 440 | 300 | 11 | 18 | 120.8 |
H400×400 | 400 | 400 | 13 | 21 | 171.7 |
H400×200 | 400 | 200 | 8 | 13 | 65.4 |
H450×200 | 450 | 200 | 9 | 14 | 74.9 |
H488×300 | 488 | 300 | 11 | 18 | 124.9 |
H500×200 | 500 | 200 | 10 | 16 | 88.1 |
H588×300 | 588 | 300 | 12 | 20 | 147.0 |
H700×300 | 700 | 300 | 13 | 24 | 181.8 |
H800×300 | 800 | 300 | 14 | 26 | 206.8 |
H900×300 | 900 | 300 | 16 | 28 | 240.1 |
項 目 | 允許偏差 | 圖 示 | |||
高 度H (按型號) | <400 | ±2.0 | |||
≥400~<600 | ±3.0 | ||||
≥600 | ±4.0 | ||||
寬 度B (按型號) | <100 | ±2.0 | |||
≥100~<200 | ±2.5 | ||||
≥200 | ±3.0 | ||||
厚度 | t1 | <5 | ±0.5 | ||
≥5~<16 | ±0.7 | ||||
≥16~<25 | ±1.0 | ||||
≥25~<40 | ±1.5 | ||||
≥40 | ±2.0 | ||||
t2 | <5 | ±0.7 | |||
≥5~<16 | ±1.0 | ||||
≥16~<25 | ±1.5 | ||||
≥25~<40 | ±1.7 | ||||
≥40 | ±2.0 | ||||
長度 | ≤7m | +60 0 | |||
>7m | 長度每增加1m或不足1m時,正偏差在上述基礎上加5mm | ||||
翼緣斜度T | 高度(型號)≤300 | T≤1.0%B。但允許偏差的最小值為1.5mm。 | |||
高度(型號)>300 | T≤1.2%B。但允許偏差的最小值為1.5mm。 | ||||
彎曲度 | 高度(型號)≤300 | ≤長度的0.15% | 適用于上下、左右大彎曲 | ||
高度(型號)>300 | ≤長度的0.10% | ||||
中心偏差S | 高度(型號)≤300且寬度(型號)≤200 | ±2.5 | |||
高度(型號)>300或寬度(型號)>200 | ±3.5 | ||||
腹板彎曲度W | 高度(型號)<400 | ≤2.0 | |||
≥400~<600 | ≤2.5 | ||||
≥600 | ≤3.0 | ||||
端面斜度 e | e≤1.6%(H或B),但允許偏差的最小值為3.0mm |
牌號 | 元素,% | 碳當量(CEV)% | |||||||||
C | Si | Mn | P | S | Ni | Nb | Mo | Ti | B | ||
Q460EM | ≤0.20 | ≤0.50 | ≤1.70 | ≤0.025 | ≤0.020 | ≤ 0.80 | ≤0.07 | ≤0.4 | ≤ 0.20 | ≤0.004 | ≤ 0.48 |
牌號 | 拉伸試驗a | V型沖擊試驗Akv/J | |||
屈服強度ReL/Mpa | 抗拉強度Rm/MPa | 斷后延伸率 (A)/% | 試驗溫度 ℃ | 縱向 | |
Q460EM | ≥460 | 540~720 | ≥17 | -50 | ≥34 |
序號 | 檢驗項目 | 取樣數量 | 取樣方法 | 試驗方法 |
1 | 化學分析 | 1(每一爐罐號) | GB/T 222 | GB/T 223 |
2 | 拉伸試驗 | 1/批 | GB/T 2975 | GB/T 228 |
3 | 沖擊試驗 | 3/批 | GB/T 2975 | GB/T 229 |
河南鋼達貿易有限公司 技術服務